Friday, December 07, 2007

Daggerboard profile transferred to foam block

I got to work on the living room floor tonight tracing the profile information that is available . I traced the information using carbon paper where possible and a long ruler for marking measured lengths where required.

Note that I first made a positioning error on the lower daggerboard profile.

The high density insert areas are marked out and I guess the next step is to cut them out.

Wednesday, December 05, 2007

Daggerboard construction starts with the construction of the basic foam block.

It's too cold to work in the garage so I decided to build up the daggerboard from two layers of 25mm thick corecell A450 offcuts from Noahsmarine in the basement. The offcuts are in 46 in lengths so joining the foam sheets was the first task to complete. If you look closely below you can see that I use sharp little tooth picks to help keep the foam sheets in line while the polyurethane glue cures.

Once the foam sheets are together I've used an weak epoxy resin cabosil mixture to glue the two sheets together to get to the required 50 mm thickness for the daggerboard. You will note that I have laid down a sheet of 9 oz glass cloth down what will be the trailing edge of the board. This will be to provide extra strength in this thin section.

Then they are clamped together.

Next is the transfer of the daggerboard profile to the foam, and the areas that require high density inserts.

Sunday, December 02, 2007

First float half lamination complete, hull re-oriented and quickly weighed

The first float half outer hull sheathing is now complete.

And the float frames have been reversed and the float re-oriented for the next half.

We did a quick weigh with the two bathroom scales, with two people with and without holding the float. It looks like the float weighs about 90lbs with the other half and the deck still to be laminated. There is still a chance I can meet Ian's theoretical weight of 112lbs for a float ready for painting.

Monday, November 26, 2007

Laminate quality part 2

Well I guess practice does make you better. I removed the peel ply tonight on section 2 for inspection and it is even better than the first section. The white peel ply and the plastic sheet really allow you to 'have at' all the problem areas. It is a combination of visibility and the freedom to work the whetted cloth without damaging it.

In terms of cloth to resin ratio I can report the following

  1. Each layer of the 8.9 oz/sq yd cut to an area of 50" x 35" weighs about 12 oz. So with the two layers I am applying there is ~ 24 oz of cloth involved.
  2. I mixed up about 29-30 oz of resin and there was a little left over, that I did not weigh. I am assuming I applied about 27-28 oz of resin onto the surface of the float foam and the cloth. I also suspect that with this wet technique there is alot of foam surface roughness that has to be filled up to get good adhesion.
  3. I weighed the peel ply after removing it tonight and compared it to a similar unused sheet of the white peel ply. Unused the 3 oz peel ply weighs 4.95 oz. After peeling it with the epoxy saturating the material it weighed 7.25 oz. So there is about 2.25 oz of epoxy in the peel ply.
I can conclude that I am approaching a 1:1 resin to cloth ratio. Perhaps with vacuum bagging you can do better, but after looking at this latest result I am very very happy with what I am achieving.

It is really a huge thing for me. I was very concerned about my ability to produce a high quality outer hull laminate.

Sunday, November 25, 2007

Laminate quality

I'm posting a couple of pictures that show the surface features of the laminate. It is not easy to get the camera to focus at this distance. I'm interested in getting some comments on the quality of laminate that I am producing and the 'dry' or 'air bubble' features that I am seeing.


Above is a good area.

Do I need to repair an area like this? The glass is hard, well adhered to the foam and there is no obvious bubble dome. Comments?


Here is the next section with peel ply and plastic on the glass.
I've purchased some white peel ply and I have to admit I like it a lot better than than the black. Visibility as the peel ply goes transparent is obviously much better. I'm just doing one more 50" length section on the hull until I have a better handle on the technique.

Thursday, November 22, 2007

Carbon fiber mast poll

I've removed the poll as it was clear that there is definite interest in a group purchase of the 35' F22R carbon fiber mast. Ian Farrier has also made a comment on Nov. 10th in the yahoo F-boat forum regarding a group purchase of F22-R masts and a special Al extrusion specifically for the F22.

"If you don't need your F-22 mast immediately then I would advise holding off for a while. I will be getting to mast options soon, and with so many boats in the pipeline it may be possible to do a bulk buy on F-22R carbon masts for the benefit of all builders.

I will also be looking at designing and extruding a specific aluminum mast for the F-22, one that has the optimum properties and least amount of weight for that purpose. The numbers could be such that a container load of masts can then be shipped to major population areas keeping prices to a minimum.

I used to arrange mast group buys in Brisbane for the Trailertri series, and at that time was able to supply mast sections for around $150 each. Will not get even close to that now, but I think it will be possible to do a lot better than builders buying individually."
I for one will wait and see what he will come up with.

Sunday, November 18, 2007

Starting float outside laminations

It is time to start the propane heater if I am going to do any laminating in November.

The float has been sanded, filled,sanded, filled.........as much as I can. It is as prepared as I can make it.

I have decided to follow the following strategy for laminating the float exteriors.

  1. Lay the first layer of the 8.9 oz 7781 cloth down. The bolt is 50 inches wide so I will be running a number of widths down the length of the hull. This allows the finished edges to run vertically up the hull.
  2. I require to lay two layers of the cloth to make the specification of 16-18oz fiberglass weight. This gives me an opportunity to offset each layer 3" down the length of the hull and have only two layers of cloth everywhere. No need for rebates to compensate for extra layers of fiberglass.

Getting the two layers of cloth wetted out and lying smooth is always the hardest work. Here I have just laid out the second layer of style 7781 e-glass cloth.

After smoothing out the plastic on the peel ply I used masking tape to hold the edges of the plastic over the gunwale, keel and bow tight curves.


The temperature is about zero outside but on the plastic it looks like it is almost 15 degrees celcius. Warm enough for epoxy to cure.

Seven hours later the resin has cured sufficiently to relese the plastic. It just lifts off , no pulling or peeling, leaving a very smooth glossy peel ply and laminate. This technique certainly saturates the peel ply with excess resin.
I'll update when the peel ply comes off. I had planned to go farther down the hull in this work session. But as the fates have it I ran out of peel ply. So, if it looks as good with the peel ply off I'll be full speed ahead when I get more supplies.

Update:
Pictures with the peel ply off. Superb adhesion with no air bubbles causing the cloth to lift. There are still areas that are a bit dry. I am not expert enough to know if this is a problem.